反応 #3552771
関連文献 (1)
openreactiondata ↗doi:10.6084/m9.figshare.5104873.v1; patent:US07875208B2
反応条件: temp:0.00; pressure:0.00; stir:; See reaction.notes.procedure_details.
実験手順: 48 g of sodium styrenesulfonate (SSNa) (available from Sigma-Aldrich Corp.) and 2.5 g of pentafluorostyrene (PFS) are fully dissolved in 0.6 L of dimethylsulfoxide (DMSO) with heating. Then, 0.3 g of azobisisobutyronitrile (AIBN) is added dropwise to the DMSO solution. The monomers are polymerized for 24 hours or more. The polymerization is carried out varying the content of pentafluorostyrene (PFS) (5, 10, and 20 wt %). The reaction product is allowed to sit at ambient temperature. Then, a precipitate is colleted from the reaction product and filtered with a filter to obtain a poly(styrenesulfonate-pentafluorostyrene) copolymer {P(SSNa-co-PFS)). with heating The monomers are polymerized for 24 hours or more to sit at ambient temperature filtered with a filter
ソース ID: ord-b573e7de2ab64d38b3c0d5c4cd27df0a